    Mechanical
    Compression set 55.0 % ASTM D395 70℃, 22hr
    Tensile strength at break 14.7 MPa ASTM D412
    Elongation at break 516.0 % ASTM D412
    Tear strength 77400.0 N/m ASTM D624
    Tensile modulus 7.06 MPa ASTM D412 100%
    Shore hardness 89.0 ASTM D2240 Shore A
    Compression set 70.0 % ASTM D395 120℃, 70hr
    Physical
    Density 1.39 ~ 1.41 g/㎤ ASTM D1505
    Specific gravity 0.95 ASTM D792
    Intrinsic viscosity [eta] 0.78 ~ 0.82 dl/g ASTM D4603
    Acetaldehyde content Max. 1.0 ppm LC method
    Moisture content Max. 1000.0 ppm LC method
    Thermal
    Melting temp 245.0 ~ 251.0 ˚C ASTM D3418
    Other
    Fluid resistance-Weight change 2.0 % ASTM D471 50% NaOH, 25℃, 168hr
    Fluid resistance-Weight change 0.0 % ASTM D471 50% NaOH, 25℃, 168hr
    Shore hardness after aging 95.0 ASTM D2240 Shore A, 150℃(168hr)
    Tensile strength at break after aging 11.76 MPa ASTM D412 150℃, 168hr
    Elongation at break after aging 430.0 % ASTM D412 150℃, 168hr